Part 6 · Bambu X2D + AMS 2 Pro

TPU & flexible filaments on the X2D

Flexible filament is the one material family where the X2D's dual-nozzle design has a hard rule: TPU runs on the left (main) nozzle only. This page shows the feed paths Bambu supports, how to load and set up each hardness, and how to combine soft and rigid plastics into gaskets, grips and overmolded parts.

IntermediateX2D + AMS 2 Pro⏱ 30 min read
What you will learn

Which hotend sizes work for TPU 85A, 90A and 95A HF, why the right nozzle is off limits, how to route TPU (direct, top holder, Feed Assist Module, AMS), starting settings, how to dry and store it, which plates and glue to use, how to mix TPU with rigid plastics, and how to fix common faults.

Source and honesty note

Hotend compatibility, feed-path, temperature, drying and plate recommendations on this page are taken from Bambu Lab's X2D TPU guide. Retraction, speed, flow and design numbers that the guide does not state are labeled typical and are starting points to verify with a test print. Hardness grades are always printed on the spool: trust the spool first.

1. The rules of TPU on the X2D

TPU (thermoplastic polyurethane) is rubbery; it compresses and buckles when pushed, which is why feed path and speed matter more than any slicer trick. Bambu's X2D guidance boils down to five rules:

  1. Left (main) nozzle only.The auxiliary (right) extruder is a stepper on the rear panel with a 525 mm PTFE feed path; its feed resistance is too high for TPU, so Bambu does not support it. In the compatibility chart every TPU is marked not available on the right nozzle, and "TPU for AMS" is marked not recommended.
  2. Match the hotend to the hardness.See the table below. A 0.2 mm hotend is not recommended for any TPU.
  3. Keep the volumetric speed limit at the default.Do not raise speed to "make it fast".
  4. No chamber heating.Use the Strong Cooling air mode (the same as PLA).
  5. Place the model at the middle-front of the plate to reduce friction in the PTFE tube.
print area (schematic) Left / maindirect driveTPU ✓ Right / auxremote extruderTPU ✗ External spool /top holder Feed Assist Module(optional) AMS (TPU for AMS)main nozzle only All TPU paths end in the left nozzle
Figure 1. All supported TPU feed options end at the left nozzle. The right nozzle is off limits, regardless of hardness.

Which hotend for which TPU?

TPU type0.20.40.60.8High-flowRecommended feed
TPU 85A✗✗✓✓⚠ HF 0.6/0.8, ✗ HF 0.4Top spool holder or Feed Assist Module
TPU 90A✗✓✓✓⚠ with HFTop spool holder or Feed Assist Module
TPU 95A HF✗✓✓✓✓ (works on HF)External spool
TPU for AMS✗✓✓✓✓ (works on HF)Can go in the AMS (main nozzle)

✓ available, ⚠ use with caution, ✗ not available. From Bambu's TPU guide and compatibility chart. Because TPU 85A is not available on 0.4 mm, a plan for 85A means fitting a 0.6 or 0.8 mm hotend first (both nozzles must match for dual-nozzle jobs).

TPU and the Filament Track Switch

The track switch (sold separately) is not suited to TPU. Bambu states that TPU, PA-CF and similar are not supported through it, and "TPU for AMS" is marked as highly not recommended with it fitted. If you own a switch, disable it for a TPU job or use the direct external path.

2. Feed paths in detail

A soft filament needs a short, straight, low-friction path to the extruder gears. The X2D guide describes the following options.

TPU 95A HF · external spool

Recommended for TPU 95A HF. The spool sits on the external holder and loads through the left extruder inlet via a short (about 175 mm) PTFE tube. Move the spool base to the right side and do not install the holder reversed.

TPU 90A / 85A · top mount

Use a top-mounted spool holder (the same size as the P2S/P1S top holder, available as a MakerWorld model) or the TPU Feed Assist Module. Softer TPU needs less friction than the standard path allows.

TPU Feed Assist Module

Works inside an enclosed chamber; uses short (about 160 mm) PTFE pieces and a 4-pin to 6-pin adapter. It can be paired with the AMS HT TPU bypass port, in which case the AMS HT acts only as a dry box for the spool.

TPU for AMS

This specific filament type can feed from the AMS to the main nozzle. Do not use standard AMS routing for softer TPU 85A/90A; Bambu advises avoiding TPU, TPE and PVA in a standard AMS because of the bending path.

Short, straight (top holder) spool extruderinlet (L) Low friction, no sharp bends → TPU does not buckle. Long, curved (standard AMS path) AMS 2 Pro inlet More friction and bends: soft TPU can fold or stall.
Figure 2. Why soft TPU wants a straight, short path. The right-hand route is acceptable only for the "TPU for AMS" filament type that Bambu validated.

Loading TPU from the top holder (documented sequence)

  1. Open the toolhead coverand disconnect the main PTFE tube from the extruder.
  2. Heat the main hotend to 250 °Cand insert the filament into the extruder inlet.
  3. Tap load slowly.Do not tap repeatedly: soft TPU wraps around the gears if it is pushed too fast.
  4. Unload the same way at 250 °C; do not pull cold.
Before you start a TPU job

If the hotend has printed other materials, run Nozzle Cold Pull Maintenance from the Toolbox (cold pull with PLA or PETG 2 to 3 times; never with a fiber-reinforced filament), and check the extruder gears and filament cutter for wear. Dirt and residue are the most common reason soft TPU grinds.

3. Starting settings: 95A, 90A and 85A

Starting points only

Items marked doc come from Bambu's TPU guide. Items marked typical are common practice for TPU on direct-drive printers and must be verified with a test print on your spool.

SettingTPU 95A HFTPU 90ATPU 85A
Nozzle0.4–0.8 mm doc0.4–0.8 mm doc0.6–0.8 mm doc
Nozzle temperatureper spool label225 °C doc225 °C doc
Bed30–35 °C doc30–35 °C doc30–35 °C doc
Chamber / air modeNo chamber heating; Strong Cooling doc
Volumetric speed limitKeep the preset default; do not raise doc
Flow dynamics calibrationAuto or Off doc
RetractionShort and slow, e.g. a fraction of the PLA value; may be off for 85A typical
Outer wall speedFar below PLA; slower for 85A typical
Part fanModerate; reduce for small layers if layers stick typical
PlacementMiddle-front of the plate doc
Relative speed / retraction PLAhigh TPU 95A HFmoderate TPU 90Alow TPU 85Alowest Conceptual trend only. Softer = slower feeding, shorter retraction. Bambu says to keep the default volumetric limit.
Figure 3. The softer the TPU, the gentler the feed. Heights show direction of change, not measured values.

Why TPU speed is limited by flow, not motion

TPU is compressible: when the extruder pushes, some of the push compresses the filament and the PTFE guide tube instead of reaching the nozzle. The faster you go, the more of it is lost, until the filament buckles or the gear slips. A volumetric speed limit caps the plastic volume per second to a level the path can deliver. Raising it is the single most common cause of failed TPU prints; Bambu's own advice is to leave it at its default.

Why slower is also better visually

Flexible filaments hold pressure in the nozzle like a squeezed sponge. Slow, constant flow keeps pressure stable, which is also why Bambu advises Auto or Off for flow-dynamics (pressure compensation) on TPU rather than aggressive tuning.

4. Drying and storage

TPU absorbs moisture; wet TPU pops, strings and prints with a rough, bubbly surface. Bambu's documented guidance:

Dry70 °C oven or75–85 °C bed, 8 h Checkspool swellsfits the holder? Storesealed, desiccant< 20 % RH Load250 °C, slowtaps only Print Documented values from Bambu's X2D TPU guide.
Figure 4. The TPU spool lifecycle from the documentation: dry, check, store, load, print.

5. Build plate and glue

PlateTPU?Glue stick?
Cool plateNot recommended doc—
Engineering plateYes docRecommended
Smooth PEI / high-temp plateYes docRecommended
Textured PEIYes docNo glue: it causes excess adhesion
Release tip

If a smooth-plate TPU print grips too hard, let the bed cool, flex the plate gently and peel from a corner; do not pry with a scraper while the part is warm (typical practice).

6. TPU with rigid plastics: interfaces and multi-material tricks

The X2D's two nozzles make soft-plus-rigid prints practical, but the TPU-left-only rule shapes every plan. A few patterns work well.

🔧 TPU as a support interface (and rigid as TPU's support)

A support interface is the thin layer between support and model. A flexible interface can peel off a rigid part cleanly because it stretches rather than snaps; a rigid support under a TPU part gives a stable, flat base that TPU cannot provide by itself. In both cases the support and the model are different materials that do not bond strongly (typical expectation; test your pair). The slicer needs the interface and body materials assigned to different filaments, and the nozzle assignment must respect the TPU rule.

A · TPU interface under a rigid part rigid support (PLA / PETG) TPU interface rigid part TPU stays on the main nozzle only. B · Rigid support under a TPU part rigid raft / support TPU part Rigid layer gives a flat base; TPU prints on top.
Figure 5. Two interface combinations. The material that is difficult to remove should be the one that forms the clean break.
Adhesion between TPU and other plastics is material-dependent

TPU bonds strongly to some plastics and barely to others; Bambu's TPU guide does not publish a bond chart. Run a small peel test with your exact pair before designing around either outcome (see exercise X-6 and X-9).

Where each filament goes

PlanTPURigid materialNotes
Dual-material, one jobLeft nozzle, external/top holder pathRight nozzle, via an AMS wired to the right-hand inletRigid on the auxiliary is limited to 200 mm/s and about 1000 mm/s². Check that your AMS pairing allows the assignment in Studio's grouping dialog.
Dual-material, TPU for AMSLeft nozzle, from AMS (TPU for AMS type)Same nozzle, filament change, or other AMS to rightWithout a track switch the AMS side stays fixed; plan the slots carefully.
Two jobs, then assembleLeft nozzle, own jobAny nozzleMost robust: print each material at its own ideal settings and snap or glue together.
AMS 2 Pro (right side) 1PLA 2PETG 3spare 4spare External spool (direct path) TPU 95A HFshort PTFE to left extruder inlet Right / auxrigid, ≤ 200 mm/s Left / mainTPU only Assemblyrigid frame +TPU seal Example slot plan; the AMS must be set up on the side that feeds the right nozzle (see AMS Setup).
Figure 6. A dual-material slot plan for a rigid housing with a flexible seal: TPU direct to the left nozzle, rigid plastics from the AMS to the right nozzle.
Multi-material tricks that usually pay off

(1) Print the rigid part of the assembly first, so the TPU prints on top of a stable shell (typical). (2) Add a 0.2–0.4 mm design gap or interlocking lip between TPU and rigid regions instead of relying on chemical adhesion (typical). (3) Keep TPU layers away from long travel moves; combine TPU regions into one tool change per layer. (4) Use a tall, wide prime tower when switching to or from TPU, because TPU leaves pressure in the nozzle. (5) Avoid rapid alternations: each tool change adds time and risk.

7. Gaskets, seals and overmolding-style printing

Gaskets

A printed gasket works by being compressed between two faces. Design for a modest compression (typical 10–30 % of the gasket thickness, depending on hardness) and for a groove that holds the gasket in place. Softer TPU (85A) seals more easily but is harder to print; 90A or 95A is more forgiving (typical). Print gaskets flat on the plate so the layer lines run along the seal, not across it, and use 100 % infill or a high wall count for a continuous, non-porous seal.

Uncompressed lid TPU gap above the lid Compressed lid TPU The gasket squashes and fills the gap; the groove keeps it located.
Figure 7. A gasket in a groove: design for modest compression and give the soft part somewhere to expand.

Overmolding-style printing

Printing a soft grip, bumper or seal directly onto a rigid part imitates overmolding. It works best when the two materials are mechanically locked (undercuts, holes through which the TPU flows, dovetails) and not only chemically bonded. On the X2D, TPU on the left nozzle and the rigid core on the right nozzle in one job is the more advanced route; the safer route is to print the rigid core first, pause or re-load, then print the TPU region. Reduce travel across the TPU regions, and avoid TPU on the very first layer of a plate containing other materials if the TPU is only a small portion (typical).

rigid core TPU grip soft region dovetail locks the TPU Mechanical interlock + a small gap/lip is more reliable than relying on sticking alone. Checklist • undercut or hole to lock • 0.2–0.4 mm design gap (typical) • TPU region ≥ 2 mm thick • keep TPU on left nozzle • test a small piece first
Figure 8. Overmolding-style design: lock the soft material mechanically, then verify the combination with a small test.

8. Test models worth printing first

rear of plate front of plate (preferred for TPU) avoid: long travel, more PTFE friction cube tower gasket bridge hinge place here
Figure 9. A single test plate laid out at the middle-front, as Bambu recommends for TPU.

9. Troubleshooting cards

Gear grinding / wrap Cause: loading too fast,worn gears, dirt. Fix: slow load taps at 250 °C,check gears and cutter,cold pull first. Stringing Cause: wet filament, hot nozzle,no retraction. Fix: dry 8 h, shorter travel,test small retraction. Under-extrusion Cause: speed too high, pathfriction, partial clog. Fix: keep default volumetriclimit, front placement, shorterPTFE, clean nozzle. Bubbles / popping Cause: moisture. Fix: dry (70 °C oven or 75–85 °Cbed, 8 h), store < 20 % RH. Sticks too hard Cause: glue on textured PEI,cool plate wrongly used. Fix: no glue on textured PEI;avoid the cool plate. Blob on the nozzle Cause: residue or oozing from aprevious material. Fix: clean the nozzle and sock,enable clumping detection.
Figure 10. Six common TPU faults, their usual causes and first fixes. Details for hotend cleaning are on the maintenance page.

10. Flexible-specific warnings from the documentation

Do not

Choosing a hardness

Shore hardness (the "A" number) measures how deep a standard probe sinks into the material: lower means softer. The X2D guide covers three grades plus a special AMS-friendly type, and the choice is a trade between feel and printability:

95A (HF)

Firmest. Easiest to push through a path and the only one Bambu recommends from a plain external spool. Good for belts-like parts, bumpers, protective feet and anything that must keep its shape under load.

90A

A middle ground. More cushion than 95A, still workable on 0.4 mm. Needs the top-mounted holder or the Feed Assist Module for a gentle path.

85A

Softest in the guide and hardest to feed. Needs a 0.6 or 0.8 mm hotend and the top holder or Feed Assist Module. Choose it for soft seals and comfort grips only when 90A is not soft enough.

Start firm, go softer later

Learn the geometry, retraction and plate behavior on 95A HF. Once your design works, swap to a softer grade, which usually needs a slower print, a bigger nozzle and a better feed path. A design that fails at 95A will not succeed at 85A.

Softer by design: geometry before grade

On the X2D, moving to a softer grade is not just a filament swap. TPU 85A needs a 0.6 or 0.8 mm hotend, and for a dual-nozzle job both sides must match; 90A and 85A also need the top holder or the Feed Assist Module instead of a plain external spool. Before paying that cost, make the firm, easy grade feel softer with geometry. Walls, infill and shape change how a part squashes far more than a few points of Shore hardness.

Need it softer? Climb only as far as you must 1 · Fewer walls,less infill95A HF, 0.4 mm 2 · Compliant shaperibs, hollow profile,thinner sectionstill 95A HF, 0.4 mm 3 · TPU 90A0.4 mm still OKtop holder orFeed Assist Module 4 · TPU 85A0.6 or 0.8 mm hotend(both sides fordual-nozzle jobs)top holder or FeedAssist Module cost and print difficulty rise to the right →
Figure 11. Steps 1 and 2 keep the hardware you already have. The hotend and feed-path requirements in steps 3 and 4 are from Bambu's TPU guide (table in section 1).
LeverFeels softer when…Watch out
Wall countFewer walls (2 instead of 4)The biggest single effect; change it first (typical)
Infill densityLower density, for example 10–20 % instead of 40 %Too low and the top surface sags into the infill
Infill patternGyroid or cubic for even squash in every directionGrid and rectilinear are springier in one direction (typical)
ShapeRibs, slots or a hollow tube profile instead of a solid blockThin ribs need at least two line widths to print reliably
Sealing partsNot applicable: gaskets need solid, non-porous wallsFor a seal, choose the grade first (section 7), not low infill

The general version of these rules, with examples, is on flexibles & specialty filaments. Print one small sample per setting, squeeze them side by side, and write the settings on each with a marker.

Slicer workflow for a TPU job

  1. Select the hotend sizein the printer preset that matches what is installed (0.6 or 0.8 for 85A).
  2. Pick the TPU filament presetand confirm it is assigned to the left nozzle in the filament list. If Studio proposes the right nozzle, use Custom grouping and move it.
  3. Choose the plateto match the surface (textured PEI without glue, or engineering/smooth plate with glue).
  4. Position the modelat the middle-front, then set flow dynamics to Auto or Off.
  5. Check the speedshown for outer walls; do not raise volumetric speed.
  6. Sendand watch the first layers on the camera: a clean, slightly squished first layer is the sign you are on track.

Design tips for flexible parts

More general joint and fastener rules are in joints and fasteners and tolerances and fits.

Key takeaways

Practice and next

Try X-6 (TPU + rigid combo) and X-7 (drying with a weigh-in). The gasket and housing recipe is in recipes; background on flexible materials is on flexibles and specialty.