Cheat sheets
Twenty-one compact, printable sheets for the printer bench: temperatures, drying, layer and nozzle rules, strength settings, tolerances, hole and thread sizes, G-code, a troubleshooting one-pager, calibration order, first-layer checks, formulas, an X2D quick-card, build plates and a maintenance schedule. All values are typical starting points; your printer, filament and slicer have the last word.
- 1 Materials
- 2 Drying
- 3 Layers & nozzles
- 4 Strength
- 5 Tolerances
- 6 Holes & threads
- 7 Pockets
- 8 G-code
- 9 Troubleshooting
- 10 Calibration
- 11 First layer
- 12 Formulas
- 13 X2D
- 14 Shortcuts
- 15 Plates
- 16 Starting values
- 17 Post-processing
- 18 Safety
- 19 Pre-flight
- 20 Terms
- 21 Maintenance
Each sheet fits on roughly half a page. Print the ones you use most and pin them next to the printer. Where a number is a range, start in the middle and adjust. Always follow the filament maker’s label when it differs from the table.
1 · Material temperature & speed quick table
| Material | Nozzle °C | Bed °C | Chamber / enclosure | Part fan | Typical speed | Notes |
|---|---|---|---|---|---|---|
| PLA | 190–230 | 35–65 | Open or vented | 80–100 % | 60–300 mm/s* | Softens near 55–60 °C |
| PLA+ / silk / matte | 200–235 | 45–60 | Open | 60–100 % | 40–200 mm/s | Silk: slower, hotter |
| PETG | 230–260 | 70–85 | Open or warm | 30–60 % | 40–200 mm/s | Strings; glue stick on smooth plates |
| ABS | 240–270 | 90–110 | Enclosed, 40–65 °C | 0–30 % | 40–200 mm/s | Fumes; ventilate |
| ASA | 245–275 | 90–110 | Enclosed, 40–65 °C | 0–30 % | 40–200 mm/s | UV stable |
| TPU 95A | 210–235 | 30–60 | Open | 30–100 % | 15–60 mm/s | Short filament path; low retraction |
| PA6 / PA12 (nylon) | 250–290 | 80–100 | Enclosed, warm | 0–30 % | 30–120 mm/s | Dry before use; glue stick |
| PC / PC blends | 260–300 | 100–120 | Enclosed, hot | 0–20 % | 30–100 mm/s | High warp risk |
| PET-CF / PA-CF / PA-GF | 260–300 | 80–110 | Enclosed, warm | 0–30 % | 30–120 mm/s | Hardened nozzle |
| PVA / BVOH (support) | 180–220 | 45–60 | Open, dry | 50–100 % | 20–60 mm/s | Very hygroscopic |
* Speed limited by volumetric flow (sheet 12) and printer acceleration. High-flow hotends allow the upper end; standard hotends plan on 12–20 mm³/s for PLA. Use the filament label as primary source.
2 · Drying table
| Material | Temperature | Time | Store at humidity | Sensitivity |
|---|---|---|---|---|
| PLA | 45–55 °C | 4–8 h | < 30 % RH | Low to medium |
| PETG | 60–65 °C | 4–8 h | < 20–30 % RH | Medium |
| ABS / ASA | 70–80 °C | 4–6 h | < 30 % RH | Low to medium |
| TPU | 50–65 °C | 6–10 h | < 20 % RH | High |
| PA (nylon), PA-CF | 80–90 °C | 8–12 h | < 10–15 % RH | Very high |
| PC | 80 °C | 8 h | < 20 % RH | High |
| PVA / BVOH | 45–55 °C | 6–12 h | < 10–15 % RH | Extreme |
Cardboard spools survive ~50–60 °C; plastic spools usually 65–80 °C. A dryer with a lower maximum (the AMS 2 Pro tops out at 65 °C) cannot dry nylon or PC fully: use a dedicated dryer or a hot-air filament dryer for those. Signs of wet filament: popping or hissing, steam, bubbles, stringing, rough surface. See drying & storage.
3 · Layer height & nozzle rules of thumb
| Nozzle | Layer height | Line width | Best for |
|---|---|---|---|
| 0.2 mm | 0.05–0.15 | 0.22–0.26 | Miniatures, fine text |
| 0.4 mm | 0.08–0.30 | 0.42–0.50 | General purpose |
| 0.6 mm | 0.15–0.45 | 0.62–0.75 | Fast, strong parts |
| 0.8 mm | 0.20–0.60 | 0.82–1.0 | Large, draft, vases |
- Layer height ≈ 25–75 % of the nozzle diameter. Below 25 % the plastic is squashed and unreliable; above 75 % layer bonding suffers.
- Line width ≈ 100–125 % of nozzle diameter; wider lines are stronger and faster.
- Halve the layer height → double the time (roughly) and hide more layer lines.
- Strength: thicker layers and wider lines usually bond better than tiny ones.
- Details smaller than the nozzle cannot be printed; keep features ≥ 1× line width, walls ≥ 2 lines.
4 · Infill & walls for strength by application
| Application | Walls | Infill | Top / bottom layers | Orientation tip |
|---|---|---|---|---|
| Decorative / display | 2 | 5–10 % gyroid | 4 / 3 | Best-looking face up |
| Prototype / fit test | 2–3 | 10–15 % grid/cubic | 4 / 4 | Fast layers, 0.2–0.28 mm |
| Everyday functional (brackets, clips) | 3–4 | 20–30 % gyroid/cubic | 5 / 4 | Layers perpendicular to the main load |
| Load-bearing / mechanical | 4–6 | 30–50 % | 6 / 5 | Never load layers in tension |
| Threaded or insert bosses | 4+ | 40–100 % near the boss | 5 / 5 | Axis of screw ∥ layers is weaker |
| Watertight / pressure | 4–6 | 40–100 % | 6 / 6 | Hot nozzle, slow, high flow stability |
| Flexible (TPU) | 2–3 | 10–20 % gyroid | 4 / 4 | Low speed |
| Vase / spiral | 1 continuous | 0 % | Solid base | 0.6–0.8 mm nozzle for strength |
Remember: walls add more strength than infill. Adding a wall usually beats adding 20 % infill. Fine-tune with local modifiers (extra walls only around holes).
5 · Tolerance cheat sheet for design
Clearance is the hole diameter minus the shaft diameter in CAD (diametral); the per-side gap is half of that. The classes match Tolerances & fits. Values assume a calibrated 0.4 mm nozzle printer; measure a test coupon on your machine and adjust.
| Fit | Clearance (diametral) | Gap per side | Use |
|---|---|---|---|
| Press | 0.00 to +0.10 mm | 0–0.05 mm | Dowel pins, bushings, magnets, bearings in a tight seat (check by test print) |
| Snug / transition | +0.10 to +0.20 mm | 0.05–0.10 mm | Lid plugs, alignment pins; holds without glue |
| Slip | +0.20 to +0.30 mm | 0.10–0.15 mm | Slide-on caps, stacked parts, general assembly |
| Sliding / running | +0.30 to +0.40 mm | 0.15–0.20 mm | Hinge pins, drawers, rotating knobs |
| Loose | +0.40 to +0.60 mm | 0.20–0.30 mm | Large parts, hot-chamber materials, lids that must always close |
| Print-in-place (separate parts printed together) | 0.60–1.00 mm | 0.30–0.50 mm; down to 0.2–0.25 on tuned printers | Chains, hinges, captive balls |
- Minimum wall: 2 line widths (0.8–1.2 mm for a 0.4 nozzle).
- Smallest hole that prints reliably: about 1.5–2 mm (drill out for accuracy).
- Smallest pin: 2–3 mm diameter.
- Text: ≥ 1 mm line thickness, 0.6 mm relief height.
- Max unsupported bridge: 20–30 mm (longer with tuning).
- Overhang limit: ≈ 45° without supports; 60° with good cooling.
- Chamfer instead of fillet at the bottom edge (0.5 mm × 45°) to defeat elephant foot.
- Holes shrink by 0.1–0.3 mm; add compensation in CAD.
Deeper treatment: tolerances & fits.
6 · Hole & thread sizes (M2–M8)
| Screw | Clearance hole (close / loose) | Self-tap pilot hole | Tap drill (cut thread) | Heat-set insert hole* | Min. wall around insert |
|---|---|---|---|---|---|
| M2 | 2.2 / 2.4 mm | 1.6–1.7 mm | 1.6 mm | 3.0–3.2 mm | 1.5 mm |
| M2.5 | 2.7 / 2.9 mm | 2.0–2.1 mm | 2.05 mm | 3.6–3.8 mm | 1.6 mm |
| M3 | 3.2 / 3.4 mm | 2.5–2.7 mm | 2.5 mm | 4.0–4.2 mm | 1.6–2 mm |
| M4 | 4.3 / 4.5 mm | 3.3–3.5 mm | 3.3 mm | 5.4–5.6 mm | 2 mm |
| M5 | 5.3 / 5.5 mm | 4.2–4.4 mm | 4.2 mm | 6.3–6.5 mm | 2.4 mm |
| M6 | 6.4 / 6.6 mm | 5.0–5.2 mm | 5.0 mm | 7.8–8.0 mm | 3 mm |
| M8 | 8.4 / 8.8 mm | 6.8–7.0 mm | 6.8 mm | 9.8–10.0 mm | 4 mm |
* Insert hole depends on the insert brand and length; always check its datasheet and print a test. Make the hole 0.5–1 mm deeper than the insert so melted plastic has room.
- Self-tapping into plastic: works for M3 and larger with 2+ mm of wall; fine for a few assembly cycles only. Use inserts for repeated use.
- Printed threads: M8 or larger work well; model with 0.2–0.4 mm clearance and print vertically. Smaller threads are better tapped or insert-based.
- Taps in plastic: go slow, back out often, no oil on nylon-bound parts (use water or dry).
7 · Screw head, nut and magnet pockets
| Size | Socket-head counterbore (Ø × depth) | Hex nut trap (across flats × thickness) | Washer Ø |
|---|---|---|---|
| M2 | 4.2 × 2.2 mm | 4.2 × 1.8 mm | 5.2 mm |
| M3 | 6.0 × 3.2 mm | 5.7 × 2.6 mm | 7.2 mm |
| M4 | 7.6 × 4.2 mm | 7.2 × 3.4 mm | 9.2 mm |
| M5 | 9.2 × 5.2 mm | 8.2 × 4.2 mm | 10.2 mm |
| M6 | 10.8 × 6.2 mm | 10.2 × 5.2 mm | 12.5 mm |
| M8 | 13.6 × 8.2 mm | 13.2 × 6.7 mm | 17 mm |
Magnet pockets (disc magnets)
- Pocket diameter = magnet diameter + 0.1–0.2 mm (press fit) or + 0.3 mm (glued). Depth = magnet height + 0.1 mm.
- Leave 0.4–0.6 mm (2–3 layers) of plastic between the magnet and the mating face; thinner is stronger but fragile.
- Pause the print at the pocket’s top layer, insert the magnet, resume. Check polarity first with a marked reference magnet.
- Secure with a drop of cyanoacrylate or epoxy for anything that is pulled hard.
- Keep magnets away from pacemakers, credit cards and electronics; heat above ~80 °C weakens common neodymium magnets.
8 · G-code quick reference
| Command | Meaning |
|---|---|
G0 / G1 X Y Z E F | Move (G1 extrudes if E given); F = feed rate in mm/min |
G2 / G3 | Arc clockwise / counter-clockwise |
G4 P1000 | Dwell 1000 ms |
G28 | Home axes |
G29 | Auto bed leveling (Marlin-like firmware) |
G90 / G91 | Absolute / relative positioning |
M82 / M83 | Absolute / relative extruder mode |
G92 E0 | Set current extruder position to 0 |
M84 | Disable stepper motors |
| Command | Meaning |
|---|---|
M104 S220 | Set nozzle temperature (don’t wait) |
M109 S220 | Set nozzle and wait |
M140 S60 | Set bed temperature |
M190 S60 | Set bed and wait |
M106 S255 | Part fan on (0–255); M107 off |
M220 S100 | Speed factor (%) |
M221 S95 | Flow factor (%) |
M204 P500 | Set print acceleration |
M600 | Filament change / pause (firmware dependent) |
M117 text | Show a message on the LCD |
Firmware-specific commands (pressure advance M900 on some firmware, SET_PRESSURE_ADVANCE in Klipper, AMS commands on Bambu machines) vary. Check your firmware before editing start or end G-code. More in G-code & firmware.
9 · Troubleshooting one-pager (symptom → fix)
| Symptom | Try first | Then |
|---|---|---|
| Stringing / oozing | Dry filament | Lower temp 5–10 °C; tune retraction |
| First layer not sticking | Wash plate | Lower Z offset slightly; slow first layer; warmer bed |
| Warping | Brim, close the enclosure | Reduce fan; raise bed temp |
| Under-extrusion / clicking | Raise temp 5–10 °C | Cold pull; slow down; check flow limit and gears |
| Over-extrusion / blobs | Flow −2–5 % | Calibrate pressure advance; move seam |
| Gaps in top surface | More top layers (5+) | More infill; reduce speed |
| Layer splitting | Hotter nozzle | Lower fan; enclose; slower |
| Ringing | Lower outer-wall acceleration | Input shaping; belts; stable table |
| Sagging overhangs / bridges | More cooling | Slower; lower temp; supports |
| Layer shifts | Check belts, collisions | Lower acceleration; check pulleys |
| Holes too small / dimensions off | Calibrate flow | Hole compensation; test coupon |
| Bubbles, popping, hissing | Dry filament | Store sealed with desiccant |
| Spaghetti | Stop print | Fix adhesion; brim; clean nozzle |
Full gallery with illustrated causes and fixes: troubleshooting. Five checks for any failure: first 5 checks.
10 · Calibration order
Calibrate in this order; each step depends on the previous ones.
11 · First-layer one-pager
- Plate washed (soap, then IPA); not touched afterwards
- Correct plate for the material
- Nozzle clean, no blob; filament purged
- Auto-leveling / Z offset calibrated
- First layer height 0.2–0.3 mm, speed 20–50 mm/s
- Bed temperature right for the material (sheet 1)
- Watch the first 3 minutes of every print
- Too high: separate round lines, gaps, peeling.
- Good: lines slightly flattened, touching, smooth.
- Too low: ridged, translucent, rough, ripples, elephant foot.
- Adjust Z by ±0.02 mm at a time.
12 · Unit conversions & useful formulas
| Convert | Formula |
|---|---|
| mm ↔ inch | 1 in = 25.4 mm |
| mm/s ↔ mm/min | × 60 (80 mm/s = 4800 mm/min) |
| °C ↔ °F | °F = °C × 9/5 + 32 |
| g ↔ oz | 1 oz = 28.35 g |
| kg ↔ lb | 1 kg = 2.205 lb |
| mm³ ↔ cm³ | 1 cm³ = 1000 mm³ |
| Filament Ø 1.75 mm cross-section | ≈ 2.405 mm² |
| Filament Ø 2.85 mm cross-section | ≈ 6.38 mm² |
- Volumetric flow (mm³/s) = line width × layer height × speed. Example: 0.42 × 0.20 × 150 = 12.6 mm³/s.
- Max speed = max flow ÷ (line width × layer height). With 15 mm³/s: 15 ÷ (0.42 × 0.20) ≈ 178 mm/s.
- Filament length (mm) = volume (mm³) ÷ 2.405 (1.75 mm filament).
- Mass (g) = volume (cm³) × density (g/cm³).
- Print time ≈ path length ÷ average speed, plus accelerations, travel and layer overhead (often +20–40 %).
- Cost = grams × (price per kg ÷ 1000) + energy + wear.
| Material | Density g/cm³ | 1.75 mm: g per meter | Meters per 1 kg |
|---|---|---|---|
| PLA | 1.24 | ≈ 3.0 | ≈ 335 |
| PETG | 1.27 | ≈ 3.05 | ≈ 327 |
| ABS / ASA | 1.04–1.07 | ≈ 2.5–2.6 | ≈ 390–400 |
| TPU | 1.21 | ≈ 2.9 | ≈ 340 |
| Nylon (PA) | 1.14 | ≈ 2.7 | ≈ 365 |
| PC | 1.20 | ≈ 2.9 | ≈ 345 |
Try these formulas interactively in the calculators.
13 · X2D quick-card
Enclosed dual-nozzle CoreXY printer. Values below follow the manufacturer’s documentation as of writing; confirm against the current manual and firmware.
| Item | Value |
|---|---|
| Build volume (main / left nozzle) | 256 × 256 × 260 mm |
| Aux (right) nozzle only | 235.5 × 256 × 256 mm |
| Max nozzle temperature | 300 °C |
| Actively heated chamber | up to 65 °C |
| Aux nozzle limits | ≈ 200 mm/s, ≈ 1000 mm/s² acceleration |
| Standard nozzle | 0.4 mm; optional kit with 0.2 mm and 0.6 mm |
| Default plate | Textured PEI, 256 × 256 mm |
| Filtration | Pre-filter + HEPA H12 + activated carbon |
| AMS 2 Pro | 4 slots; drying to 65 °C max; 6-pin cable |
- Main nozzle (left) prints the model: direct-drive servo extruder, full speed.
- Aux nozzle (right) is fed by a separate extruder with a long PTFE path: use slower speeds, longer retraction, official filament where possible, and ideal for support material or a second material.
- Flow-dynamics calibration applies to the main nozzle only; the aux nozzle needs its own, much larger K value.
- Chamber: keep PLA open/cool (vent the chamber); heat the chamber for ABS, ASA, PC, nylon and CF materials.
- Drying in the AMS 2 Pro is limited to 65 °C: fine for PLA, PETG, TPU; use a dedicated dryer for nylon and PC.
Full details: X2D overview, dual-nozzle printing, AMS 2 Pro, maintenance & troubleshooting.
14 · Slicer-agnostic shortcuts & mouse
Most slicers (Bambu Studio, OrcaSlicer, PrusaSlicer, Cura) share these conventions. Menus differ; check yours under Help → Keyboard shortcuts.
| Action | Typical keys |
|---|---|
| Undo / redo | Ctrl+Z / Ctrl+Y (or Ctrl+Shift+Z) |
| Copy / paste / delete | Ctrl+C / Ctrl+V / Del |
| Select all | Ctrl+A |
| Arrange objects | A (in many slicers) |
| Slice | Ctrl+R (varies) |
| Standard views | Number keys 0–6 (iso, top, bottom, front, rear, left, right) |
| Mouse | Action |
|---|---|
| Left drag on empty space | Orbit the view |
| Right or middle drag | Pan the view |
| Scroll wheel | Zoom |
| Click object | Select; Ctrl/Shift adds to selection |
| Drag object | Move on the plate |
| Layer slider | Scrub through layers in preview |
Scrub the layer slider before you start: look for floating islands, missing supports, odd seam positions and gaps in thin walls. Thirty seconds here saves hours.
15 · Build plates & adhesion picks
Match the plate to the material first; only then reach for glue, brims or bed temperature. Bed temperatures are on sheet 1.
| Plate | Best for | Watch out |
|---|---|---|
| Textured PEI | PLA, PETG, ABS/ASA; nylon with glue; most everyday prints | Matte bottom; hides small first-layer flaws |
| Smooth PEI | Glossy bottoms in PLA, PETG, ABS/ASA | PETG can tear the coating: use glue stick as a release layer |
| Cool Plate (low-adhesion) | PLA, delicate or low-temperature prints | Not for high-temperature materials |
| Engineering / high-temp plate | PA, PC, PET-CF, hot-bed ABS, with glue | Needs the right glue for each material |
| Glass (borosilicate) | Very flat parts in PLA or PETG | Needs glue or hairspray for most plastics |
| Material | Start on | Aid |
|---|---|---|
| PLA | Textured or Cool Plate | Usually none; a clean plate matters most |
| PETG | Textured PEI | Glue stick as release on smooth PEI |
| ABS / ASA | Textured or engineering plate | Glue; brim; closed, warm chamber |
| Nylon (PA, CF/GF) | Engineering plate | Nylon glue; filament must be dry |
| PC | Engineering plate | Strong glue; brim; hot chamber |
| TPU | Smooth or textured PEI | Glue as release (it sticks very well) |
- Clean: warm water and dish soap removes skin oil; an IPA wipe between prints keeps it clean. Do not touch the print area.
- Release: let the plate cool, then flex it. A part that will not come off a cold flexible plate needs glue as a separator next time, not more force.
- Order of fixes: clean plate → right plate → Z-offset → bed temperature → brim → glue. Change one at a time.
16 · Starting values: retraction, supports, bridges, cooling
Treat these as starting points for a first test, not final answers. Always change one value at a time and print a small test.
| Setting | Direct drive | Bowden |
|---|---|---|
| Retraction distance, PLA / PETG | 0.4–1.2 mm | 3–6 mm |
| Retraction distance, TPU | 0–1 mm | Avoid retraction; slow down |
| Retraction speed | 25–45 mm/s | 30–60 mm/s |
| Z hop | 0–0.4 mm (only if needed) | 0.2–0.4 mm |
| Travel speed | 150–500 mm/s | 100–250 mm/s |
| Pressure advance (K) | Calibrate per nozzle and filament; do not copy numbers between printers | |
| Setting | Starting value |
|---|---|
| Support overhang threshold | 45–55° |
| Support top Z gap | 0.1–0.2 mm (0.2–0.3 for PETG) |
| Support interface layers | 2–3 |
| Support pattern | Tree for organic shapes; grid/lines for flat ones |
| Bridge speed / flow | 20–40 mm/s; flow 0.85–0.95 |
| Bridge fan | 100 % |
| Overhang fan | 100 % for PLA; low for ABS/ASA |
| Brim width | 5–8 mm (10+ for warp-prone parts) |
17 · Post-processing quick picks
| Sanding step | Grit | Purpose |
|---|---|---|
| Rough | 120–180 | Remove blobs and support scars |
| Medium | 240–320 | Flatten layer lines |
| Before primer | 400 | Prepare for filler primer |
| Between coats | 600–800 (wet) | Smooth primer |
| Polish prep | 1000–2000 (wet) | Gloss finish |
| Joining | Best for |
|---|---|
| Cyanoacrylate (super glue) | PLA, PETG, ABS quick joints; add baking soda for gaps |
| Two-part epoxy | Strong joints, mixed materials, nylon |
| Solvent welding (acetone / DCM / THF types) | ABS/ASA (acetone); handle solvents with great care |
| Plastic welding / hot air | Large repairs; needs practice |
| Heat-set inserts | Screws that must be reused (sheet 6) |
Work outdoors or with strong ventilation, wear nitrile gloves and eye protection, and keep solvents away from flames. Sand wet or use a mask: plastic dust, especially carbon-fiber, should not be inhaled. See post-processing.
18 · Safety one-pager
- Never leave a printer running where you cannot reach it or hear a smoke alarm; install a smoke detector in the room.
- Ventilate when printing ABS, ASA, nylon, PC and resins; consider an enclosure with filtration.
- Nozzle (up to 300 °C) and bed (up to 110 °C and above) cause instant burns; wait for cooling before touching.
- Power off and unplug before opening electronics or the hotend.
- Use flush cutters and scrapers away from your body; wear eye protection when removing supports.
- Do not use printed parts for food contact, structural safety or electrical insulation without proper evaluation.
- Keep a fire extinguisher (ABC or CO₂) accessible; never use water on an electrical fire.
More: safety & workspace.
19 · Pre-flight checklist
Model & slicer
- Model is manifold, oriented for strength and supports
- Right printer, nozzle size and plate selected
- Filament profile matches the spool in the machine
- Walls, infill, top/bottom set for the application (sheet 4)
- Supports and brim set where needed
- Layer preview checked (no gaps, no islands)
Printer
- Plate clean, correctly seated
- Nozzle clean; no old plastic on the bed or purge area
- Filament dry, spool turning freely, no tangles
- Enough filament for the whole print (weight estimate + 10 %)
- Chamber/lid set for the material; printer ventilated
- Camera or monitoring on; stay near for the first layer
If anything looks wrong during the first layer: stop, fix, restart. It is cheaper than any other time to fix it.
20 · Slicer terms in one line
| Term | Plain meaning | Turn it when… |
|---|---|---|
| Wall loops / perimeters | Number of outlines printed around each layer | You need strength or watertightness |
| Sparse infill | Internal lattice that fills the part | You need stiffness or support for top layers |
| Top / bottom shells | Solid layers above and below the infill | Top is rough or has gaps |
| Seam | Where each outline starts and ends | You want to hide the vertical line |
| Retraction | Pulls filament back before travel moves | Stringing or oozing appears |
| Pressure / flow dynamics | Compensates for pressure lag in the nozzle | Corners bulge or gaps follow corners |
| Flow ratio | Multiplier on extruded volume | Walls look too thick or too thin |
| Brim / skirt | Extra lines around the base / purge line | Warp-prone or tall, thin parts |
| Ironing | Extra smoothing pass on top surfaces | You want a glossy flat top |
| Z hop | Lifts the nozzle during travel | Nozzle scars the top surface |
| Arc fitting | Replaces tiny line segments with arcs | Smooth curves and smaller files |
| Wipe tower / prime tower | Purge area for material changes | Multi-color or multi-material prints |
| Adaptive layer height | Thinner layers on curves, thicker on flats | You want speed with smooth details |
| Modifier | A region with its own settings | One area needs extra walls or density |
More terms in the glossary and slicer settings.
21 · Maintenance intervals
A condensed version of the maintenance schedule. Print hours matter more than calendar time: a printer running every day reaches “monthly” sooner. Follow your printer maker’s schedule where it differs.
| Interval | Tasks | Time |
|---|---|---|
| Every print | Plate clean and seated; nozzle free of old plastic; right filament loaded and dry; purge area clear | 1 min |
| Weekly | Wash the plate (soap, then IPA); vacuum debris from chamber and rails; wipe rods; check desiccant; look over fans and the toolhead cable | 10 min |
| Monthly | Thin film of lubricant on rails and rods; belt tension and teeth; clean extruder gears; tighten screws; blow dust from fans; check PTFE tube ends | 40 min |
| Quarterly | Grease lead screws; inspect or replace the nozzle (sooner with abrasives); check filters; inspect heater and sensor wiring; refresh desiccant | 1 h |
| Yearly | Replace worn PTFE tubes, silicone sock, wiper and cutter; deep clean; check fans and bearings; update firmware and back up profiles; replace a worn plate | 2 h |
| Nozzle | Rough lifetime |
|---|---|
| Brass, normal filaments | 3–6 months of regular use |
| Brass, abrasive filaments | Days to a couple of spools (avoid) |
| Hardened steel | Many months to years |
- Signs it is due now: new noises, layer shifts, ringing, under-extrusion that calibration does not fix, a first layer that suddenly varies.
- Keep a log: date, print hours, task, result. It turns “it got worse” into “it got worse after the nozzle change”.
- Power off and let the hotend cool before working on it.
Start from the table values, calibrate in order, change one variable at a time, keep filament dry, and use the troubleshooting sheet before blaming the printer. Print this page and keep the sheets you use next to the machine.