Part 2 · Materials

Filament overview & comparison

Learn what is actually on the spool, why plastics behave the way they do when heated and cooled, and how to pick the right material from a field of dozens, using charts, ladders and one decision flowchart.

Beginner → Advanced⏱ 35 min read
What you will learn

🔰 What filament actually is

Filament is thermoplastic that has been melted, extruded through a precise die, cooled, and wound onto a spool as a long, thin, round “wire”. An FDM (fused deposition modeling, also called FFF) printer pulls it off the spool, pushes it into a heated nozzle, melts it, and lays it down line by line and layer by layer. Because the plastic is a thermoplastic, it softens when heated and hardens when cooled, again and again. That is the only reason the process works, and it is also why a printed part can soften in a hot car.

Almost all consumer printers, including the Bambu Lab X2D, use filament with a nominal diameter of 1.75 mm. A second standard, 2.85 mm (often called “3 mm”), exists for a few older or industrial machines. The two are not interchangeable, so always check what your printer accepts.

Flange (cardboard or plastic) Wound filament (~1 kg) Core / hub Spindle hole typical Ø 200 mm layers wound side by side hole ~ 50–55 mm Cross-section (magnified) Ø 1.75 mm nominal typical tolerance ±0.02 to ±0.05 mm dashed: out-of-round (ovality) error
Figure 1. A spool and the filament’s cross-section. Tolerance describes how much the average diameter may drift; ovality describes how far from a perfect circle the wire is. Both change how much plastic leaves the nozzle.

Diameter and tolerance

The extruder meters plastic by length, not by volume. The slicer assumes a diameter (usually 1.75 mm) and computes how many millimeters to feed. If the real wire is 1.80 mm, the cross-sectional area is about 6% too large, and so is the amount of plastic extruded. That shows up as slightly over-extruded, bulgy surfaces. A thin spot at 1.70 mm gives the opposite: gaps and weak walls. Good filament holds ±0.02 mm; budget filament is often ±0.05 mm; anything wider is a risk. A calibrated flow ratio per material (see Calibration playbook) absorbs the average error but not diameter swings along the spool.

1.75 mmstandard diameter
±0.02–0.05typical tolerance (mm)
1 kgcommon spool net weight
~330 mlength of 1 kg of PLA at 1.75 mm
Length per kilogram

Density sets the length: PLA (1.24 g/cm³) gives roughly 330 m per kg, PETG (1.27) about 320 m, ABS (1.04) about 400 m, and carbon-fiber nylon (around 1.1–1.2) 340–370 m. Light plastics like ABS and PP go further per spool, which is why price per kg is not the same as price per part.

The spool

The spool is not just packaging: it is part of the system. Its core diameter determines how tightly the filament is bent. Stiff materials like PC, PA-CF and PLA-CF dislike tight cores and can snap while being unrolled. The spool’s flange, hole size and width decide whether it fits an AMS, a dryer or a side-mounted holder. Refill spools without a reel exist for the Bambu ecosystem; you reuse a reel and save plastic and money. A spool’s weight label includes only the plastic. The empty reel weighs 150–250 g, which matters when you weigh a spool to estimate what is left.

Color, pigments and additives

A “pure” polymer is typically translucent or milky. Color comes from pigments or dyes compounded into the plastic before extrusion. Additives change behavior as well:

Property modifiers

Impact modifiers (rubber particles) make “Tough PLA”; plasticizers soften; nucleating agents speed crystallization (sharper detail, less warp in some PLA); flame retardants make V-0 grades.

Fillers and fibers

Chopped carbon or glass fiber (stiffness, low warp, abrasive), wood flour, ground metal, stone powder, glow pigment (strontium aluminate, abrasive), magnetic or conductive particles.

Process aids

Lubricants and flow improvers for high-speed PLA, anti-oxidants and stabilizers against heat degradation, UV stabilizers in ASA.

Visual effects

Silk (shiny, usually PLA with a modifier), matte (mineral fillers), sparkle, galaxy, marble, dual-color and gradient wraps. They may print at different settings than the base polymer.

Two spools of “PLA” from different brands can therefore differ more than two different polymers from the same brand. Pigment matters too: black and white are often noticeably different in flow and strength from natural or other colors, and carbon-black pigment can change heat absorption. Always treat a new brand, and even a new color, as a new material to tune (see calibration).

🔧 Polymer science in plain language

A plastic is a polymer: a very long molecular chain built from thousands of repeating units. How those chains are arranged and how they move when heated explains stiffness, heat resistance, shrinkage, clarity, chemical resistance and even how hard the material is to print.

Amorphous vs semi-crystalline

Chains either stay in a random tangle (amorphous) or partly fold into tidy, tightly packed regions called crystallites (semi-crystalline). Real plastics are a spectrum, but the two families behave differently when cooled.

Amorphous Random coil · no sharp melting point Semi-crystalline crystallite crystallite Ordered islands + tangled links · sharp melting point
Figure 2. In amorphous plastics (PLA as printed, PETG, ABS, ASA, PC) the chains stay random. In semi-crystalline plastics (nylon, PP, PEEK, PPS, PET) part of the chain packs into ordered crystals that act like tiny reinforcing anchors.

Amorphous

Softens gradually over a range of temperature. Shrinks little (0.3–0.8%), warps moderately, bonds nicely between layers. Often transparent-capable. Typical: ABS, ASA, PC, PETG, PCTG, HIPS, PEI, PVA (partly).

Semi-crystalline

Stays stiff above its glass transition until close to the melting point, then turns thin and watery. Shrinks strongly as crystals form (1–2% and more), so warping is common. Better chemical, fatigue and wear resistance. Typical: PA6/PA12/PA66, PP, PET, PPS, PEEK, POM, PLA (when annealed or nucleated).

Glass transition (Tg) and melting point (Tm)

The glass transition temperature (Tg) is not melting. It is the temperature range where the chains in the amorphous regions start to wiggle freely, and a hard glassy solid turns rubbery. A part made of an amorphous plastic loses most of its stiffness near Tg, which is why a PLA part (Tg about 55–65 °C) sags in a sun-baked car even though PLA does not melt until about 150–180 °C. Semi-crystalline plastics also have a Tg but their crystals keep them partly stiff until the melting temperature (Tm), the point where crystals dissolve.

Stiffness (log scale) Temperature → Tg Tg Tm Glassy: hard, stiff Rubbery plateau (amorphous: soft, sags) Semi-crystalline: crystals hold it up Melt print temperature is far above both Amorphous (e.g. ABS, PETG) Semi-crystalline (e.g. PA, PP)
Figure 3. Schematic stiffness-versus-temperature curves (not measured data). Amorphous plastics collapse at Tg, semi-crystalline ones keep a reduced but useful stiffness until Tm. Fiber fill raises the plateau further, which is why CF-nylon holds shape far above plain nylon.
HDT: the practical number

Datasheets often quote HDT (heat deflection temperature): the temperature at which a standard bar under a small load bends by a fixed amount. It is a handy comparison, but it depends heavily on load (0.45 vs 1.8 MPa), print orientation, infill and annealing. Treat HDT as a ranking, not a guarantee, and test your own part at the real temperature with the real load.

Crystallization, shrinkage and warping

Every plastic shrinks as it cools. Semi-crystalline plastics shrink more because the chains pack closer when they crystallize. In a print, the top layer is hot while the layer beneath is already cold and rigid. As the top layer cools it wants to contract but is held by the cold layer. The result is internal stress that pulls the part’s edges upward. That curl is warping. Adhesion to the build plate fights it; heat (a warm bed, a warm chamber) reduces the temperature difference that drives it.

1 · Layers cool and contract Build plate hot: wants to shrink cold: already rigid 2 · Stress lifts the corners Build plate lift lift corners curl off the plate
Figure 4. Warping is trapped shrinkage. The larger the temperature gap between new and old layers, and the more the material shrinks, the larger the curl. Large, flat, sharp-cornered parts in ABS, PA and PC are the classic victims.

Hygroscopy: plastics that drink water

Many polymers attract water vapor from the air (hygroscopic). Nylon, PVA, BVOH and TPU absorb it fast and in large amounts; PETG, PC, and PLA absorb less but still enough to matter. When wet filament enters the hot zone, the water flashes to steam, which makes hissing, popping, tiny bubbles, stringing and rough surfaces, and in the worst case hydrolysis, which permanently cuts the polymer chains (PLA, PETG, PET and PA are all vulnerable). The details, humidity targets and drying charts are in Drying & storage.

1. Water absorbed into the polymer 2. Heater block: water flashes to steam 3. Steam bubbles in the melt 4. Bubbles burst: pops, strings, rough layers Nylon / PVA / TPU: very fast · PETG / PLA: slower but real
Figure 5. Why wet filament misbehaves. It is not the water’s mass but its sudden expansion into steam that disrupts the melt. Long-term hydrolysis also shortens polymer chains, which makes parts brittle.

Layer adhesion and anisotropy

A printed part is made of lines welded to lines. Inside a layer the plastic is continuous and molecules are oriented along the path, so the part is strong in X and Y. Between layers, the weld depends on how hot the surfaces still were when they touched. This makes parts anisotropic: strength depends on direction. Pulling across layers (the Z direction) usually yields only a fraction of the in-plane strength, commonly 30–70%, and less for cold, fast prints. Materials that need a hot chamber (PA, PC, ABS) get much better inter-layer welds when printed warm, which is a major reason enclosed, actively heated chambers exist. See Strength & orientation for design rules.

Pull along layers (X/Y) Load carried by continuous lines Strength ≈ 100% Pull across layers (Z) layer line splits Strength often 30–70% (colder = lower)
Figure 6. Layer lines are the weak planes. Orient parts so loads run along the lines, add walls rather than infill where strength matters, and print semi-crystalline or high-temperature materials warm.

📊 The master comparison

The two tables below cover 29 material families. The first table tells you how to print each one; the second tells you what the printed part can do. All figures are typical ranges for commercial filaments; formulations vary by brand, so always start from the spool label or your slicer’s vendor profile and tune from there. Scroll sideways on a phone.

Table A · How to print it

MaterialNozzle (°C)Bed (°C)Chamber / enclosureDry before useHardened nozzle?PrintabilityPrice tier
PLA190–23035–65None; open lid is better45–55 °C · 4–8 hNo$
PLA+ / Tough PLA200–23545–60None45–55 °C · 4–8 hNo$–$$
PLA-CF210–24045–60None45–55 °C · 6–8 hYes$$
PETG230–26070–85Optional; avoid drafts60–65 °C · 4–8 hNo$
PETG-CF240–27070–80Optional60–65 °C · 6–8 hYes$$
PCTG240–27070–90Optional65 °C · 6–8 hNo$$
ABS240–26090–110Enclosure needed70–80 °C · 4–6 hNo$
ASA240–27090–110Enclosure needed70–80 °C · 4–6 hNo$–$$
HIPS230–25090–110Enclosure needed60–65 °C · 4–6 hNo$$
PC260–300100–120Enclosed + warm chamber80 °C · 8 hNo$$
PC-ABS250–280100–110Enclosure needed70–80 °C · 6 hNo$$
PA6 / PA66250–29070–100Enclosed; warm chamber helps80–90 °C · 8–12 hNo (yes if CF)$$
PA12230–26050–90Enclosure needed70–80 °C · 8 hNo$$$
PAHT (high-temp nylon)270–30080–100Enclosed + warm chamber80–90 °C · 8–12 hUsually CF-filled$$$
PA-CF260–30080–100Enclosed + warm chamber80–90 °C · 8–12 hYes$$$
PET-CF260–29070–100Enclosure recommended65–80 °C · 6–10 hYes$$$
PPS-CF300–340100–120Hot chamber; high-temp hotend100–140 °C · 8–12 hYes$$$$
PP220–25080–100Enclosure helps50–60 °C · 4–6 hNo$$
TPU 95A210–24030–60None50–65 °C · 6–10 hNo$$
TPU 85A200–23030–60None50–65 °C · 6–10 hNo$$
TPE (soft, 60A–80A)200–23030–60None50–65 °C · 6–10 hNo$$
PVA180–22045–60None45–55 °C · 6–10 hNo$$$
BVOH190–22045–60None50–60 °C · 6–10 hNo$$$
PEI / ULTEM family340–390120–160Industrial 120–180 °C chamber120–150 °C · 6 h+No (CF grades yes)$$$$$
PEEK / PEKK370–420120–150Industrial 120–200 °C chamber120–150 °C · 6 h+No (CF grades yes)$$$$$
Wood-fill190–22045–60None45–55 °C · 4–6 hAdvisable ≥0.6 mm nozzle$$
Metal-fill190–23045–60None45–55 °C · 4–6 hYes$$–$$$
Glow-in-the-dark200–23045–60None45–55 °C · 4–6 hYes (abrasive)$$

Price tier: $ = cheapest common filament; $$$$$ = specialty industrial. Printability (5 dots = easiest) assumes a well-tuned enclosed printer, not a bare open-frame machine.

Table B · What the printed part can do

MaterialStrengthStiffnessHeat (approx. Tg / HDT)ImpactUV / outdoorChemicalsTypical use
PLA55–60 °CModels, prototypes, display
PLA+ / Tough55–60 °CFixtures, snap fits, desk parts
PLA-CF55–65 °CStiff, matte brackets, drone frames
PETG70–80 °CBrackets, outdoor-light, containers
PETG-CF75–85 °CStiff functional parts
PCTG70–85 °CClear, tough, shatter-resistant
ABS95–105 °CEnclosures, automotive interior, smoothed parts
ASA95–105 °COutdoor housings, car exterior
HIPS~85–95 °CDissolvable support for ABS
PC110–140 °CTough hot parts, clear covers
PC-ABS100–115 °CTough enclosures, tooling
PA6 / PA6655–80 °C unfilledGears, bushings, hinges
PA1250–90 °C (load dependent)Living hinges, tough snap fits
PAHT~100–160 °CUnder-hood parts
PA-CF140–190 °CJigs, drone arms, tooling
PET-CF~110–180 °CRigid structural parts, low moisture sensitivity
PPS-CF200–260 °CHot, chemical, flame-retardant parts
PP~80–100 °C light loadLiving hinges, chemical tanks, ducts
TPU 95A60–80 °C softensGaskets, bumpers, phone cases
TPU 85A60–70 °C softensSeals, grips, shoe soles
TPE50–70 °C softensVery soft pads, grips
PVA≈ 75 °C (Tg); sticky when dampdissolves in waterSupport only
BVOH~60–70 °Cdissolves in waterSupport only (faster, cleaner)
PEI / ULTEM170–200 °CAerospace-grade, flame-retardant
PEEK / PEKK150–300 °CMedical, aerospace, chemical
Wood-fill50–55 °CDecor, sandable look
Metal-fill~55 °CWeighty props, polishable
Glow~55 °CNight signs, toys
Read the numbers as a ladder, not a contract

Neat polymer data sheets quote injection-molded samples. Printed parts are usually lower in strength (especially across layers) and show different heat resistance depending on infill and annealing. “Strength” above ranks printed parts against each other, not against steel.

📈 Charts at a glance

These bars summarize Table B. Heat is in approximate °C (Tg / HDT, light load); the others are relative indices for printed parts.

Heat resistance (approx. °C, light load)
PLA55–60
PETG70–80
PCTG70–85
ABS / ASA95–105
PC-ABS100–115
PC110–140
PA-CF140–190
PAHT-CF150–200
PPS-CF200–260
PEEK150–300
Stiffness (approx. flexural modulus, GPa)
TPU 95A~0.03
PA121–1.5
PETG1.8–2.2
ABS / PC2–2.4
PLA3–3.8
PLA-CF4–7
PA-CF5–8
PET-CF6–9
PPS-CF8–12
Impact toughness (index, 10 = hardest to break)
PLA-CF1.5
PLA2
PLA+4
PETG5
ASA5.5
ABS6
PC-ABS7
PA6 / PA128
PC9
TPU10
Ease of printing (index, 10 = easiest)
PLA10
PLA+9
PETG8
TPU 95A6
ABS / ASA5
PET-CF5
PA-CF4
PC / PA63
PPS-CF2
PEEK / PEI1

A property radar for four archetypes

Strength Stiffness Heat Impact Ease UV / chemicals PLA: easy and stiff, low heat PETG: the balanced all-rounder ABS: heat and toughness, harder PA-CF: strong and stiff, demanding Scale: 1 (center) to 5 (outer ring). Qualitative ranking for printed parts, not lab data.
Figure 7. No material wins every axis. Moving outward on one spoke usually costs something on another, usually “ease”. The decision comes from which axis your part cannot compromise on.

Print-temperature ladder

200 °C250 °C300 °C350 °C400 °C X2D nozzle max 300 °C ~260 °C: PTFE-lined hotend limit PVA / BVOH PLA TPU PP PETG HIPS ABS / ASA PC-ABS PA6 / PA12 PET-CF PC PA-CF / PAHT PPS-CF PEI / ULTEM PEEK / PEKK
Figure 8. Typical nozzle temperature ranges. Everything left of the dashed line is fine on a PTFE-lined hotend. Above roughly 260–280 °C you need an all-metal path, and above 300 °C a dedicated high-temperature hotend. The red line marks the X2D’s 300 °C nozzle limit; PPS and PEI-class materials are outside the printer’s rating.

🌡️ Nozzle, bed and chamber requirement matrix

Hotter materials demand more of the printer. This matrix groups materials by what hardware they need. “Warm chamber” means an enclosure that holds heat from the bed and nozzle; an actively heated chamber adds a heater and is what makes the hardest materials routine.

ClassMaterialsHotendBedChamberPart cooling
Class 1 · EasyPLA family, PVA, BVOH, TPU≤ 240 °C, any hotend25–60 °COpen or enclosed with lid openHigh (60–100%) for PLA; low for TPU
Class 2 · ModeratePETG, PCTG, PET-CF, PP230–290 °C70–100 °COptional; stable air; PP prefers warmLow to medium (20–60%)
Class 3 · EnclosedABS, ASA, HIPS, PC-ABS, PA12240–280 °C90–110 °CClosed; 40–60 °C air from the bed alone often enoughVery low (0–30%)
Class 4 · Warm chamberPC, PA6/66, PAHT, PA-CF260–300 °C all-metal80–120 °CHeated chamber 50–65 °C strongly preferredOff to low
Class 5 · IndustrialPPS-CF, PEI, PEEK, PEKK300–420 °C special hotend100–160 °CChamber 100–200 °COff
Bambu X2D + AMS 2 Pro

The X2D reaches a 300 °C nozzle and an actively heated chamber up to 65 °C, which covers Classes 1 to 4 on paper, including PC, PA and PAHT-CF. Class 5 is outside its range. See Engineering materials & chamber and Filament compatibility for what is rated on the main versus the auxiliary nozzle. The AMS 2 Pro can dry spools at up to 65 °C; that suits PLA, PETG, TPU and ABS-class drying but is below what nylon prefers (Drying & storage).

⚙️ When you need a hardened nozzle

Brass is soft. Carbon fiber, glass fiber, glow pigment (strontium aluminate), metal powders, and some stone or ceramic fills act like fine sandpaper and widen a brass orifice within a few hundred grams. A wider hole means over-extrusion, dull detail, and eventually inconsistent flow. The cure is a nozzle made of hardened steel, tungsten carbide, ruby-tipped or coated alloys. Hardened steel conducts heat less well than brass, so you typically raise the nozzle temperature by 5–10 °C and keep flow in check.

Required

All carbon-fiber and glass-fiber filaments (PLA-CF, PETG-CF, PA-CF, PAHT-CF, PET-CF, PPS-CF, ASA-CF), glow-in-the-dark, metal-filled, many “marble” or ceramic-style fills.

Recommended

Heavy glitter or sparkle, “galaxy”, some stone fills, high-percentage wood filaments (also use ≥ 0.6 mm to avoid clogs), recycled filaments with unknown fillers.

Not needed

Plain PLA, PETG, ABS, ASA, PC, TPU, PA without fiber, silk and standard colors, and most dual-color or gradient filaments.

Not every printer ships with a hardened nozzle; some official hotends and nozzle kits are compatibility-limited by material, so check the printer’s filament table before you load a fiber-filled spool (X2D filament compatibility).

🧭 Decision flowchart

Start from the job, not the material. The chart below names the best first choice for six common needs and the minimum hardware and drying each one needs.

What must the part do? Looks, models,prototypes,fit checks Tough, water-resistant, snapfits, brackets Sun, rain, UV,garden, carexteriors Hot places:80–110 °C,near motors Wear, oil, fuel,high load,gears, tools Soft, bendy,grippy, seals,bumpers PLA / PLA+silk, matte, tough PETG / PCTGPLA+ if indoors ASAPETG for light duty ABS · PC-ABSPC (hottest) PA6 · PA12PAHT / PA-CF TPU 95A / 85ATPE if very soft Any printerDry 45–55 °CBed 25–60 °C Dry 60–65 °CBed 70–80 °CUse glue stick EnclosureBed 90–100 °CVentilate Enclosure, warmchamber, dryBed 100–110 °C Dry 70–90 °CWarm chamberCF: hardened nozzle Direct driveSlow speedsDry 55–60 °C Need clean overhangs or hollow shapes?Add soluble support: PVA or BVOH (for PLA/PETG), HIPS (for ABS). Beyond 300 °C nozzle or 65 °C chamber?PPS-CF, PEI, PEEK need an industrial machine.
Figure 9. Pick by need, then check the requirements row against your hardware. If your printer misses a requirement, step left: PETG instead of ASA indoors, PLA-CF instead of PA-CF for stiffness, or a different design.

For a personalized answer, use the interactive Material picker: answer a few questions about heat, outdoors, strength and printer, and it recommends a first-choice material.

🚀 Strategy: choosing like an engineer

  1. Write the requirement listMaximum temperature in service, load type (static, impact, cyclic), environment (UV, water, oil, fuel, cleaning chemicals), contact (skin, food), and appearance. A part that “just needs to be strong” is not a requirement.
  2. Find the dominant constraintOften one property decides: heat points to ABS/PC/PA-CF, UV to ASA, flex to TPU, wear to PA, stiffness to CF-composites. Decide on that first.
  3. Check your hardwareHotend rating, enclosure, chamber heating, nozzle hardness, dryers and AMS compatibility. Step down if the printer cannot support the first choice.
  4. Pick the cheapest material that passesPLA and PETG are cheaper, faster and more forgiving. Use harder materials only where the requirement forces you.
  5. Prototype in PLA, then test the real materialUse a throwaway PLA to prove fit and geometry. Then print the final one and test it under real load and heat before releasing it.

Mini case studies

Dashboard phone mount

Summer cabin temperature can pass 70 °C. PLA would sag, PETG is marginal, so ASA (or ABS) is chosen. ASA is also UV-stable. Printed enclosed at 100 °C bed.

Garden hose connector

Outdoors, wet, UV, and some pressure: PETG works for light duty; ASA is better; nylon would absorb water and swell. Chosen: ASA with 5 walls.

Drive gear

Sliding wear and impact: PA6 or PA12 (low friction, tough); PA-CF if stiffness matters more than toughness. Needs dry filament and a warm chamber.

Common mistakes

Choosing the “strongest” filament

“Strong” depends on how a part fails. PLA has a high tensile strength but cracks under impact; PETG or nylon bends and survives. CF composites are very stiff but brittle across layers.

Ignoring creep and heat

Plastics under a steady load slowly deform (creep), and much faster when warm. A PLA hook that carries a plant pot at 22 °C can fail in sunlight months later even if it never broke on day one.

Printing fiber-filled filament in a brass nozzle

It will “work” for the first hundred grams and then slowly ruin print quality. Fit a hardened nozzle first.

Pro trick: material swap test

Print the same small functional part in two materials, then abuse them: bend, drop, heat in an oven at 60, 80, 100 °C, immerse in the real chemical. An hour of testing beats days of forum reading.

Where to go next

🟢

PLA, PETG & everyday plastics

The workhorses, in depth.

🔩

Engineering plastics

ABS, ASA, PC, nylon, composites.

🪀

Flexibles & specialty

TPU, supports, silk, wood, glow.

💧

Drying & storage

Moisture science and dryers.

🧮

Material picker

Answer questions, get a pick.

📐

Strength & orientation

Design for anisotropy.

Key takeaways